WINFLOW-SM  
AE high range water reducer (Standard Type) KSF2560


A standard lignin-based AE water reducer with naphthalene as a major component. It increases the strength of concrete by reducing the unit quantity of concrete and increases durability due to air-entraining admixtures to make dense concrete. In addition, it can be widely used for all concrete structures.

● USAGE
* Ready mix concrete plant or Batch plant field
* Concrete secondary products manufacturing plant
* General construction and civil engineering structures
* Concrete roads, runways, and bridges
* Concrete using binders (Fly Ash, Slag Powder)

● DOSAGE
* 0.3 ~0.7 wt% of total binder
* For optimal use, it is recommended to mix the actual formulation of concrete on-site in order for supervision to choose the amount of cement based on the strength and workability of the concrete based on site conditions.
* Since air-entrainment is affected by the mixing ratio, concrete materials selection, temperature, and placement methods, the amount used should be adjusted as the concrete is placed.
* Use of excessive amounts may cause problems with the concrete. Thus caution is required.

● ADVANTAGES
* The amount of cement required is reduced due to the excellent dispersion.
* Increased compressive strength due to a high water reducing ratio of 13%~18%
* Reduction in segregation of materials and concrete bleeding at high slump
* Increased resistance to freezing and thawing due to increased durability and water tightness.
* Excellent concrete properties based on binder substitution  

● PROPERTIES
* Appearance  : Dark brown liquid
* Specific gravity : 1.200±0.05 (20℃)
* pH     : 7.0±3.0
* It can be used in parallel with other admixtures.

Packing 
* 250kg/drum, Tank Lorry

MixingDesign

Class

 Gravel
Size(mm)

 W/C(%)

S/A(%)

 Unit weight (kg/㎥)

 W

 C

 S

 G

 AD

 PLAIN

 25

 65.0

 48.0

 195

 300

 873

 953

 

 WINFLOW-SM

 25

 55.3

 47.0

 166

300

 854

 970

 1.5

 WINFLOW-SM

 25

 52.7

 47.0

 161

 300

 860

 977

 2.1


TestResults

 Test Item

 KSF2560

 PLAIN

 WINFLOW-SM

 Admixture dosage (%)

 -

 -

 0.5

 0.7

 Air Content (%)

 Plain+1.0

 1.4

4.6

 4.8

Slump(㎜)

 80±10

 85

 80

 80

Water Reduction (%)

 4≤

 -

14.9

 17.4

Bleeding (%)

 100≥

100 

56.0

 53.6

 Setting Time
(Hr : Min)

Initial

  -60 ~ +90

 0

+30

+45

Final

 -60 ~ +90

 0

+35

 +45

Compressive strength ratio (%)

3Day

 125≤

 100

135

 139

7Day

 125≤

 100

128

 132

28Day

 125≤

 100

125

 129

Elongation (%)

 120≥

 -

 126

 104

Relative dynamic modulus of elasticity (%)

 80≤

 -

 97.3

 97.9


 

 Length change test           : Water curing for 7 days (20±2) and moist curing for 6 months (Temperature 20±2, Humidity 60±5%)

※ Freeze-Thaw Resistance test        : Specimen Temp. (4℃ → -18 -18℃ → 4) 200 cycles